The effects of prewash are sometimes mentioned. I was working on a development scheme for some film and needed to tame contrast.
The H&D curves presented show the film (SVEMA 42L) with and without a 3 min prewash of tempered H2O .
The gamma without prewash was 1.12 (red) and with the prewash the gamma was 1.05. The developer (T-max 1:4), temp. (24c) and time (3:00 min) were the same for both.
The effect is measurable, but subtle. About a 6% lowering of contrast.
The control strips were exposed with a Wejex sensitometer and measured with a calibrated Tobias TCX Densitometer.
The H&D curves presented show the film (SVEMA 42L) with and without a 3 min prewash of tempered H2O .
The gamma without prewash was 1.12 (red) and with the prewash the gamma was 1.05. The developer (T-max 1:4), temp. (24c) and time (3:00 min) were the same for both.
The effect is measurable, but subtle. About a 6% lowering of contrast.
The control strips were exposed with a Wejex sensitometer and measured with a calibrated Tobias TCX Densitometer.